z測試粘度,干膜厚度,外觀,酒精循環(huán)擦拭,酒精沾污測試,交叉劃格法測試附著力,鉛筆硬度和透明拉拔
zTested with six thermoplastic acrylics, Paraloid B66, Paraloid A21, NeocrylB805, Degalan M825, Degalan LP68/04 and Degalan M890
z共測試六種熱塑性丙稀酸樹脂:Paraloid B66, Paraloid A21,Neocryl B805,Degalan M825, Degalan LP68/04 and Degalan M890
zRatio of Acrylic:CAB (on solids basis) = 4:1
z丙稀酸樹脂:CAB(固體份比)= 4:1
zCoated samples flashed off for 20 minutes, baked for 15 minutes @ 70oC andaged for 24 hours before testing
z被噴涂的樣品在空氣中放置20分鐘,然后放入70oC烘箱中烘烤15分鐘,取出放置于常溫中24小時后測試
zCAB 381-20BP improves the metallic appearance of the coating
zCAB 381-20BP可提高含金屬粉涂料涂膜的外觀
zAlcohol resistance of all the coatings were not affected by the additionof CAB 381-20BP. In fact CAB 381-20BP improves the alcoholresistances of all the formulations
z加入CAB 381-20BP不會影響涂膜耐醇性。實際上,在所有配方中,CAB 381-20BP都可提高耐醇性
zTo formulate a good alcohol resistance coating, it is important tochoose a low hydroxyl value and high molecular weight CAB